1 (edited by PheonixSD3 2015-03-15 11:53:39)

Topic: Top Layer Problems

[SOLUTION] See posts 15 and 21 in this thread.

Need some help with this one.  Printing in Octave ABS. Tuned my wall thickness, did belt tension, layer height @ 0.2963mm, and general maintenance last weekend.

My top layer has been acceptable until lately when I've been trying to print an Arduino project box.  This is probably the longest top surface I've tried to print which may be why I haven't seen this until now.  There's a portion of the top layer that just does not want to print correctly.  I can't tell if it's not sticking to the lower layers (extrude temp 210C) or if it's over-extruding and squishing out the side of the layer and then warping up. (Pic below) I've tried this with 2 and 3 top layers over 25% infill and get the same thing each time.

What is going on here and what are your recommendations?

Thanks

http://i.imgur.com/mmHGPbm.jpg

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

2

Re: Top Layer Problems

First thing I'd do is print that at 100% infill.  You've already wasted more ABS than you're going to save.  Try that and let's see where it gets you.

Printit Industries Model 8.10 fully enclosed CoreXY, Chamber heat
3-SD3's & a Workbench all fully enclosed, RH-Slic3r Win7pro, E3D V6, Volcano & Cyclops Hot End
SSR/500W AC Heated Glass Bed, Linear bearings on SS rods. Direct Drive Y-axis, BulldogXL
Thanks to all for your contributions

3

Re: Top Layer Problems

Ok, trying another one now with some different settings.  I've never actually done anything at 100% before.  Will make a solid one also and report back with results - maybe tonight, maybe tomorrow morning.

Let's say this was a larger/thicker part where weight and material usage would make 100% infill unfavorable - what suggestions then?

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

4

Re: Top Layer Problems

PheonixSD3 wrote:

Ok, trying another one now with some different settings.  I've never actually done anything at 100% before.  Will make a solid one also and report back with results - maybe tonight, maybe tomorrow morning.

Let's say this was a larger/thicker part where weight and material usage would make 100% infill unfavorable - what suggestions then?

I've said it before, I'll say it again.
Master 100% infill and the rest is easy.  You will learn more about your printer than you ever thought possible.
For your question I would use at least 3 perimeters and about 50% infill.  Three bottom and top layers. 
I would use an extrusion width for first layer of .36 and same for the top.  All other layers I would use .48
It also seems that you are having some extrusion issues on infill.  That's the cause of your problem and could be as simple as slowing the speed down or dialing in your temperature a little better.

Printit Industries Model 8.10 fully enclosed CoreXY, Chamber heat
3-SD3's & a Workbench all fully enclosed, RH-Slic3r Win7pro, E3D V6, Volcano & Cyclops Hot End
SSR/500W AC Heated Glass Bed, Linear bearings on SS rods. Direct Drive Y-axis, BulldogXL
Thanks to all for your contributions

5 (edited by PheonixSD3 2015-03-14 03:15:03)

Re: Top Layer Problems

I'll post some pictures in a moment when my phone recharges (good camera is at work).  My next-to-top layer is nearly perfect as you'll see in a picture soon but what is so frustrating is that the top layer is absolute junk.  That layer (next-to-top) is at default and gcode shows it at 0.42 (same as single wall tuned). Currently I think that the extrusion width is too far from tuned values. The pic in the post above is at 105% width for top infill and the coming pic (pretty bad but enlightening) is at 80% (whice gcode indicated was 0.24mm!!).  I have just enough time to try the tuned value explicitly at 0.42mm (nope - going with Ward's suggestion) and will report on that when it is done.  Really, my gs4 was at 2% when I was last begging it to take a picture and it refused - back soon.

Thanks for the insight Ward. I'm going to hold off for just a moment to try out this line of reasoning and then I'll start seeing what 100% looks like and show any progress.

Food for thought:
I pretty much always use 3 perimeters.
I'll try the 0.36 and 0.48 on this next run.
I'm down to 40 mm/s - do you really suggest slower?

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

6

Re: Top Layer Problems

40 is slow enough try playing with the temp some sometimes hotter isn't better.  Also make sure you have no wobble in your extruder carriage.

Printit Industries Model 8.10 fully enclosed CoreXY, Chamber heat
3-SD3's & a Workbench all fully enclosed, RH-Slic3r Win7pro, E3D V6, Volcano & Cyclops Hot End
SSR/500W AC Heated Glass Bed, Linear bearings on SS rods. Direct Drive Y-axis, BulldogXL
Thanks to all for your contributions

7 (edited by PheonixSD3 2015-03-14 04:47:07)

Re: Top Layer Problems

Here's the pic of nearly perfect next-to-top and crap top layer. I stopped the print shortly into the top layer.

http://i.imgur.com/UR0ASqp.jpg

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

8

Re: Top Layer Problems

You're over-extruding, have you calibrated steps/mm and set it in EEPROM?  Should be 105-107 roughly. 
Have you calibrated single wall to .48?
If yes to both you have some mechanical slop causing your problems.

Printit Industries Model 8.10 fully enclosed CoreXY, Chamber heat
3-SD3's & a Workbench all fully enclosed, RH-Slic3r Win7pro, E3D V6, Volcano & Cyclops Hot End
SSR/500W AC Heated Glass Bed, Linear bearings on SS rods. Direct Drive Y-axis, BulldogXL
Thanks to all for your contributions

9

Re: Top Layer Problems

EEPROM is calibrated at roughly 208 steps/mm  for 1.81mm (1.75mm) Octave Orange ABS with digital calipers over 10 cm.  Single wall is calibrated to 0.42mm. I'm surprised to hear 105ish for E.  I would believe mechanical except that everything except for the top layer is manageable.

*the current print at 0.36-0.48 isn't doing so well

I'll double check E steps and let you know

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

10

Re: Top Layer Problems

*No worries about "wasting" filament as long as I get closer to a better print

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

11 (edited by PheonixSD3 2015-03-14 04:47:36)

Re: Top Layer Problems

On a side note - when I was printing at 80% top layer width it seemed as though (and really before then also) that the z-height for the top layer thickness was too high such that there was no adhesion between layers.

Also - regarding E-steps - I'm at 1/32 on the RUMBA so 208ish should be fairly close to your 105ish at 1/16.

EDIT - in the pic above, I stopped the print shortly into the top layer

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

12

Re: Top Layer Problems

You are correct about your steps. 
Something isn't moving as expected on that top layer. 
Do you have a picture of your "anti backlash z spanner"? 
I am wondering if that isn't binding during the print and as you get to that top layer it drops more than expected?

Printit Industries Model 8.10 fully enclosed CoreXY, Chamber heat
3-SD3's & a Workbench all fully enclosed, RH-Slic3r Win7pro, E3D V6, Volcano & Cyclops Hot End
SSR/500W AC Heated Glass Bed, Linear bearings on SS rods. Direct Drive Y-axis, BulldogXL
Thanks to all for your contributions

13

Re: Top Layer Problems

What is your temperature of the hotend? Had a problem myself with the top infill like your pictures. Had to set the temperature to 230 degree's. Started to go away at 223 degree's but the best was 230.

14

Re: Top Layer Problems

wardjr wrote:

You are correct about your steps. 
Something isn't moving as expected on that top layer. 
Do you have a picture of your "anti backlash z spanner"? 
I am wondering if that isn't binding during the print and as you get to that top layer it drops more than expected?

This, also what is your extrusion width for top layers? Specifically for the print pictured above.

15 (edited by PheonixSD3 2015-03-14 18:34:36)

Re: Top Layer Problems

I think I have this as solved as it can be currently.  Also, the 0.36-0.48 print turned out better than it looked at first but showed a wider range of minor defects in other layers and still had the surface problem (albeit greatly improved) - I'm thinking that these are just too far from my tuned width of 0.42mm.

Slic3r seems to have issues once I start using widths more than +-10% from my tuned single wall width - so... I have now set ALL of my widths to that (0.42mm in my case) and will slowly try changes.  The defaults and text-over suggestions were just not working out.

I should note that I still have the original extruder and 0.35mm nozzle.

Here are some pics:

First, my Anti-Backlash Z-Spanner - no indication of binding at all.  I'm thinking about updating the design soon now that I have some good CAD/CAM to work with. The current design had to be filed down on the linear shaft facing surfaces at first because the squished first layers messed up my close dimensions. Since it was then (and now) it is slightly undersized it actually gives a small clicking sound when reversing Z direction as the spanner rotates a bajillionth of a degree and switches which side of the shafts it is contacting depending on the direction of rotation.
http://i.imgur.com/BiklrAe.jpg

Second - the 0.36-0.48mm width print (0.36mm for top and bottom solids):
http://i.imgur.com/pkJdIo2.jpg

My final acceptable print at 0.42mm width for all layers:
http://i.imgur.com/m7MWJw4.jpg

I may add my current settings to this thread later tonight for posterity's sake.

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

16

Re: Top Layer Problems

Do you have a 0.4mm nozzle? If that is the case, the biggest problem is you're calibrating the wrong width. Use 0.48mm = 0.4mm*1.2  The 1.2 factor (120%) is for die swell in the nozzle. On a 0.35mm nozzle, 0.42mm = 0.35mm*1.2 is the correct value.

17

Re: Top Layer Problems

0.35mm nozzle

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

18

Re: Top Layer Problems

That is a neat design I would be curious to see that print without the z-spanner installed.  I would also like to know if you have z-lift enabled.

Printit Industries Model 8.10 fully enclosed CoreXY, Chamber heat
3-SD3's & a Workbench all fully enclosed, RH-Slic3r Win7pro, E3D V6, Volcano & Cyclops Hot End
SSR/500W AC Heated Glass Bed, Linear bearings on SS rods. Direct Drive Y-axis, BulldogXL
Thanks to all for your contributions

19

Re: Top Layer Problems

Z-lift is enabled at 0.2963mm - the same as the corrected "0.3"mm layer height. I'm definitely not taking the spanner off - at least not until I make the next one. Between the spanner and the corrected layer heights the slight z-banding I originally had (when I first got the printer) has essentially vanished - and this is with the stock SD3 5/16" Z-screw.  I have several boxes worth of upgrades sitting around (including a PEI plate, linear bearings and shafts, a Bulldog XL, and an E3D V6, and other stuff...) but as soon as they arrive, I find a good configuration with the stock setup and don't want to change anything.

In the case that I want to publish a Z-spanner on the forum - do the SD2, 3, and 4 all have the same Z arrangement? As in: shaft diameter (3/8"), distance between shafts (71.75-72mm), screw size (5/16")? I can make versions for M3 and M5 as well.  This would be at least a couple of weeks away since I have to travel for work over the next two weeks.

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

20

Re: Top Layer Problems

The 2,3&4 do have the same arrangement.  I am only wondering if that spanner isn't causing some of your top layer issues.  All of the things you are listing as problems solved by that thing are issues I don't have with out it.  I am not suggesting you remove it rather am curious to learn what is so screwed up (by SD) that it takes such extreme measures to correct. 
I am also not certain you understand the full function of z-lift.  Try setting it to zero if your machine is calibrated there is no real need to lift for every non print move.  That combined with your spanner your bed is not getting back the the correct position.  I really want to see you figure this out so at the very least set z-lift to zero and add some lube to your spanner at the guide rods and the screw.
If you'd like some help figuring the z wobble issues out let me know via PM as to keep this thread clean and on topic.

Printit Industries Model 8.10 fully enclosed CoreXY, Chamber heat
3-SD3's & a Workbench all fully enclosed, RH-Slic3r Win7pro, E3D V6, Volcano & Cyclops Hot End
SSR/500W AC Heated Glass Bed, Linear bearings on SS rods. Direct Drive Y-axis, BulldogXL
Thanks to all for your contributions

21 (edited by PheonixSD3 2015-03-15 12:22:31)

Re: Top Layer Problems

Solution below.

Um... I do consider it fixed. Thanks for the help - I definitely appreciate it.  Not trying to beat a dead horse but the spanner actually greatly improves Z repeatability and isn't binding at all.

Check out the photo of my last print in post 15 and let me know if you see anything that looks like it still needs attention. The last two pics are from different prints and the bottom one is pretty good if you ask me.  More pics - first is all of the prints (leftmost is first test print, rightmost is final good print after the bad ones), second is close up of good print.
http://i.imgur.com/QZSIwEr.jpg
http://i.imgur.com/BD4siND.jpg


[SOLUTION]
Slic3r > Advanced > Top Solid Infill was trying to use unacceptable widths.

TL/DR: Default extrusion width was bad and using the % modifier in slic3r instead of telling it real mm value hid the problem until I looked at the gcode to see that widths were very different from values acceptable for my nozzle size.

Long Story: My Slic3r was just outputting some unexpected widths and setting all widths explicitly back to my tuned width solved the wierd behavior on the top layer. I'm not sure why it was making weird widths except that I had managed to change settings enough over time that it wasn't obvious to me that it was sometimes going down to widths of 0.24mm!! No wonder it wasn't sticking to the previous layer!  History of the issue - I had changed back to all default "0" values when doing maintenence last week and instead of using explicit mm widths, I had started using % widths.  The 0.24mm was from a Slic3r>Advanced> "top solid infill" setting of 80% which means that my 100% was apparently 0.3mm width and my original (when the problem first appeared) of 105% was only 0.32mm.  This also explains why the other infill layers (which stayed at 0.42 for some reason) still looked good.



Using Z-lift just became part of my preferred settings over time to minimize knocking around any slight warped area but I'll play with it today on the next part of this project enclosure.  The next part will be the bottom which will hold the Arduino whereas the top is what you've been seeing

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r

22

Re: Top Layer Problems

Great work those slicer settings get us all sometimes wink
I just want you to know that I have no doubt that your spanner improves things.  I am more curious than anything in the way of helping others.  We see all sorts of strange problems and most of the time I can just say to a user "go ask this guy he's had and solved the same problem".  In this case it looks like a simple enough solution if it is compensating for a bent Z-rod.

Printit Industries Model 8.10 fully enclosed CoreXY, Chamber heat
3-SD3's & a Workbench all fully enclosed, RH-Slic3r Win7pro, E3D V6, Volcano & Cyclops Hot End
SSR/500W AC Heated Glass Bed, Linear bearings on SS rods. Direct Drive Y-axis, BulldogXL
Thanks to all for your contributions

23

Re: Top Layer Problems

Yep, the extrusion widths appear to have been the root cause for the above problem.

Thing is, the spanner isn't really supposed to correct a bent rod - it's only supposed to eliminate z-backlash caused by imperfect mating between the z-screw and z-nut. A bent rod is a scrap rod IMO.

I know you understand backlash so I'll leave that out. The spanner shows its advantage mostly when making extra z-movements like I do with z-lift. I don't want any uncertainty or compounding errors when moving my z.  I wouldn't think this is much of an issue for anyone not using z-lift after you get past the first layer or two.  I mostly think of it as insurance.  Between the spanner and corrected layer heights, my banding is pretty much gone.  I'm about to start the "fitness woman" to make a comparison (both use the spanner): the old one still shows minor banding with uncorrected layer heights - the new one will use corrected layer heights.

You and I are very much in agreement about correctly identifying things that help and hurt.  I've found my spanner sketchup design and will be translating it to Fusion 360 today.  When I get that made and printed I'll do a small 2 factor, 2 level DOE (4 prints) to show any differences but that is definitely at least a week away - and a new thread (I'll edit this later to include the link).

Side note - I've recently been putting a 1mm fillet or chamfer on the bottom of my designs to avoid interference from squished first layers.  It also works well to ensure proper dimensions elsewhere such as avoiding corner bulge.

SD3, RUMBA, 360W power, ABS: Glass bed + Aquanet Extra Super Hold Hairspray, Anti-backlash Z spanner, Repetier Host + Slic3r