Re: Solidoodle 3 Mods, and issues.
Ditched the glass.
in my previous glass bed measurement i let the probe reach 95C than started the clock. This time i started the clock from cold bed, all the way to the bed reached 95C on my IR gun.
Outside enclosure temp 20C
Bed Temp 20C (software)
Bed temp 20C (IR GUN)
Programmed 95C bed
2Min Soft: 57 IR gun: 45.6
4Min Soft: 75 IR gun: 59
6Min Soft: 87 IR gun:70.5
7Min Soft: 91 IR gun: 75
8Min Software programmed reached @ 95C bed temp 75C
10Min Soft: 95 IR gun: 77 (peak temp reached, 18C diff). Increase programmed temp to 110C (+15C)
15Min Soft: 110 IR gun: 93
18Min Soft: 112 IR gun: 95
Attempted to print on freshly cleaned kapton tape. Zero adhesion.
Kept the bed up to temp, and the extruder @ 200C laid out blue tape, and it stuck VERY well.
Looks like i will be trying out the painters tape from now on.
Its taking forver, but loading up 4 youtube videos that show the print and a few of my settings. Is there some type of calibration print everyone is using to adjust settings?