1

Topic: Top layer not smooth, and layers peel apart

Hello all, I believe this is my first post.  I've been working hard to get my SD3 perfect.  I'm close.

I guess I can't attach links to my pics, so I've attached pics of the problem I appear to be having (not sure if it is a problem, or not).  these are interlocking terminal blocks.

My top layer seems to have gaps, and when looked at from the side, you can tell definite layers that tend to peel apart when pried.

I am printing onto kapton tape with the extruder at 210 degrees and the bed at 90 degrees.

Any ideas?  I was attempting to make starter screw holes where I can screw in terminal screws.  It appears to work, but the holes seem to be floating.  I also expected the top layer to be a bit more filled in (particularly around the holes).

As for the layers peeling, even moderate prying with a fingernail results in a cracking and the layers splitting apart.



Thanks for your help.

Warren

Post's attachments

P1020022 (Medium).JPG
P1020022 (Medium).JPG 215.6 kb, file has never been downloaded. 

P1020025 (Medium).JPG
P1020025 (Medium).JPG 202.08 kb, 1 downloads since 2013-09-15 

P1020026 (Medium).JPG
P1020026 (Medium).JPG 193.22 kb, file has never been downloaded. 

P1020027 (Medium).JPG
P1020027 (Medium).JPG 199.92 kb, file has never been downloaded. 

You don't have the permssions to download the attachments of this post.

2

Re: Top layer not smooth, and layers peel apart

What kind of filament are you using? and also what is your print speed?

3

Re: Top layer not smooth, and layers peel apart

I'm using ABS.  This part was made using the ABS that shipped with the SD3.

My print speed is:

Perimeters: 45 mm/s
Infil: 60
Top solid infil: 50

Did I provide the right info?

Warren

4

Re: Top layer not smooth, and layers peel apart

from the looks of it, you may have an extrusion multiplayer issue, have you done flow rate calibration?

5

Re: Top layer not smooth, and layers peel apart

My $.02: do you have an enclosure around the cabinet?

I had some success by saving a new set of print settings (like "Solidoodle .2MM - three qtr speed") and slowing all the print speeds by a fourth. But that's just me. I set my bed at 100 and extruder at 200.

Also, I use an 8" square mirror I got at the craft store which works much better than Kapton and you can scrape parts off with a razor if needed. The mirror is an additional heat sink so it acts like a thermal flywheel, stabilizing the heat, although it takes longer to heat up (I let it "soak" for about five minutes after the thermistor says the bed is up to speed).

In essence, in my humble opinion, it seems like you need to give the layer underneath every chance to be warm enough and for the new layer to lay down slow enough that the two layers bond.

Finally, I get better results with the E3D hot end, about an $80 investment. But you should still get respectable results with the stock hot end.

Welcome aboard, Warren.

Robox printer, HICTOP (Prusa i3 variant) Model 3DP17 printer, ELEK 2.5W laser engraver, AutoDesk 123D Design, Windows 10

6

Re: Top layer not smooth, and layers peel apart

Extrusion multiplier + zwobble/zbacklash.

7

Re: Top layer not smooth, and layers peel apart

wsoeldner wrote:

I'm using ABS.  This part was made using the ABS that shipped with the SD3.

My print speed is:

Perimeters: 45 mm/s
Infil: 60
Top solid infil: 50

Did I provide the right info?

Warren


Hello Warren,

Just a WAG but I think I see the problem with your top layer not being smooth.

That looks as if it's infil,I don't think you're printing a top solid layer.You may have specified a "top solid infil" of .50 in your advance settings but unless you specify to slic3r the number of top solid layers to print in "layers and perimiters",you won't have a top solid layer.Set a top solid layer of two and try it again.

Post's attachments

IMG_0041.JPG 537.03 kb, file has never been downloaded. 

You don't have the permssions to download the attachments of this post.