1 (edited by lboucher26 2016-03-21 02:08:48)

Topic: Any ideas how to have more consistent diameter in this setup

Hi All

So here is my setup.
The barrel is about as insulated as its going to get with a cover plate with hold to shield the nozzle.
Nozzle is drilled to about 2.1

Filawinder and tube is mounted as secure as possible.
Pre-dried MG94 abs pellets with some colorant.
Motor and heater on different power supplies.

The filament coming out looks good, and the setup is running as reliably as i have ever been able to get.
In general, the diameter is right around 1.75 and generally stays there, but every so often it can drift up to 1.85 and down to 1.65. It seems to only do this for about 6" to a foot of length worth. If I measure the absolute worst spots its 1.61 - 1.9

The filament is generally still but i still see some sway when the filawinder turns off and on. Really can't think of a good way to stop that.

I'm running at about 194C. Speed is good, so I am thinking I will just drop temp and sacrifice speed and see what happens.
There are two fans behind the red thing, I have their voltage down to 3.3V so their is just a bit of cooling, but not enough to make the filament sway.

I kinda think its better for the first half hour or so when the filawinder tends to run consistently. Once the diameter of the spool gets bigger, it tends to start and stop. Is the firmware available for the filawinder? Maybe something can be tweaked there.

Also, the spool is really nice and tight now with the gauge adding tension, but occasionally the filament slips on itself on the spool, because the spooling isn't perfect. I'm sure that doesn't help, but I have no idea how make it spool better.

Also debating turning the fan off, and shortening the droop/temp as much as needed to get back up to 1.75... Anyone have success with no cooling on ABS?

Also, its a bit hard to really know my average diameter, as the filament really isn't circular. In the extreme I can see .05 -.1 of diameter change if i just rotate the filament.

I don't really think their is anything i can gain with automatic temp control, since the length that goes bad is only a foot or so, and the thickness gauge is about 5' away from the nozzle. So i'm left thinking the only real way to get better is to go with a direct pull setup, with a very short distance from nozzle to pull wheels, and then have active control. But i have no interest in doing that much work. In general the filament is usable and i think it kinda averages out when printing, but I would like to get a bit better.

Thanks for any thoughts.


http://soliforum.com/i/?vgQ8sYR.jpg

2

Re: Any ideas how to have more consistent diameter in this setup

194C is hot for MG94 ABS. What did you experience when starting at the recommended 180C?

Unfortunately that overdrilled nozzle will make for oversize filament at more appropriate processing temperatures.

I would also recommend lowering that sensor and placing the winder and extruder further apart if possible. A goo starting point is 35-40 inches apart, and 15-20 inches of drop.

Let me know how all that goes, we'll get it figured out!

3

Re: Any ideas how to have more consistent diameter in this setup

Thanks for the thoughts.

Moving stuff will be a good project for next weekend.

Do you mean raise the sensor? My sensor is currently about 35 inches down from nozzle, which is more than the 25 you stated.

My setup has been tweaked Alot over the past year. I did start at 180 a long time ago. I think my rate was really slow... Pretty sure I have read of others using temps in this range.... But I agree lower temp should help.

4

Re: Any ideas how to have more consistent diameter in this setup

Woops, just realized I posted a very old picture. My current setup has the sensor way lower and the filastruder is a bit farther to the right. Will post the right picture when I get home.

5

Re: Any ideas how to have more consistent diameter in this setup

Sorry, was going off the posted photo.

It is possible to use higher temperatures, but it's a bit like taking the training wheels off - at higher temperatures, everything has to be just right.

As for non-circular, that likely means either ovality induced from the cooling fan or from the nozzle orifice not being round.

The Filawinder firmware is open source and available:

http://www.soliforum.com/topic/5088/fil … mentation/

6

Re: Any ideas how to have more consistent diameter in this setup

All good. Here is the actual picture of my setup.

Thanks


http://soliforum.com/i/?AnXtCCQ.jpg

7

Re: Any ideas how to have more consistent diameter in this setup

One mod on the filawinder firmware I am considering is a minimum auto speed so it never actually fully stops. It really should never have to completely stop if ya think about it. And stopping and starting in my experience is always somewhat jerky. Inertia is always a killer when you stop. ( At least in industrial robotics.)

8

Re: Any ideas how to have more consistent diameter in this setup

I think this could be fixed by using different sized gears to change the gear ratio.  This would provide better control of the winding speed so we are not operating the motor at its lower limit. Does anyone have the scad files for the gears?

9

Re: Any ideas how to have more consistent diameter in this setup

From that updated photo, I'd try to move the winder and struder a little further apart, and the sensor up. That and I'd reduce the temperature to 185C. This will likely bring your average diameter up, I'd compensate with less cooling though you may need a non-overdrilled nozzle.

What speeds are you seeing currently, and what were you seeing at 180C?

10

Re: Any ideas how to have more consistent diameter in this setup

So i bought my filawinder about a year ago and never upgraded the firmware. Has their been any interesting additions in the past year? Is there a version log?

11 (edited by lboucher26 2016-03-28 17:30:44)

Re: Any ideas how to have more consistent diameter in this setup

Hi All

So i spent the weekend playing with the filastruder.
I was able to get things better, but still not where i think it should be.
Filawinder is now about 33 inches to the right of the extruder (cannot go any further, out of room)
Loop goes down about 30", temperature is 184.
Diameter average is about right.
Played with the firmware on the filawinder, setting min speed from 25 to 60 (which is a bit above stall speed). Also made the maximum increment of speed change 6 instead of 25. (I think i will reduce this a bit further to 4). In general, the filawinder seems to be running about as smooth as possible, introducing minimal oscillation in the filament loop. I did remove the PTFE tube loop, and now just have a straight section of tube, up to my dial caliper measurement setup, which seems to provide enough tension for the spool.
Also adjusted the guide angle step from 1.5 to 1.9. I had put in a linkage arrangement on the quide to limit overall range from +/-180 to about half that, while reducing the stress on the motor. Adjusting this angle definitely makes the spool, spool up better. Also tweaked the location of the hall transducer, i think it was bent back a bit too far from the magnet and not guite reading reliable.

Filament height sensor is slightly offset to the filawinder side.

Turned the fan off, so their is no wind affecting the filament.
At 184, my diameter is fine without it. (Although maybe i need coolant to minimize the unsteadyness of the diameter, see below)

I did manage to put 3 guides that limit movement of the filament about 6" below the nozzle. Somewhat surprised that appears to be working out just fine.

Here is a video mid way through the weekend.
https://youtu.be/wmB0wgmJpFk

So in the end, I am just barely achieving +/- 0.05 mm Every once  in a blue moon it maybe goes +/- 0.06 mm.
I can live with that, as it is usable.
However, what really surprises me is the overall behavior.
When I hear +/0.05mm, I would think 90% of the time its between +/-0.03, and maybe spends 5% of the time at the full +/-0.05mm.
What i see, is it goes back and forth between the extreme pretty fast. Like if its at +0.05, then it will likely end up at -0.05 within 6-20 seconds, and then it swings back the other way. Sometimes it will hunt around the midpoint for a bit, but I would say its swinging between the extremes at least 50% of the time.

What behaviors do others see? You really have to have a thickness gauge on it to track the diameter over time.

My thickness gauge holder does have the centerline of the pulley 0.5mm off center of the in/out hole, to provide a bit of tension. I was thinking maybe this offset causes changes in diameter to be exagurated in the gauge due to the angle of flex of the filament, but in general, the thickness gauge match my hand reading with a caliper...


Picture of guides.
http://soliforum.com/i/?mTG5E2V.jpg

12

Re: Any ideas how to have more consistent diameter in this setup

Keep in mind that 99% of the "measurements" you see on the internet for both Filastruder filament and regular filament come from calipers put on the filament a couple dozen times. If you haven't validated your measurement device's accuracy, it would be good to do so before relying on its measurements. For example, the bearings in your measurement setup might be out of round. Those chinese caliper/thickness gauge based setups are generally repeatable to +/-0.02mm, so the error you're trying to measure is pretty similar in magnitude to the error from the device itself.

By comparing your measurement setup to what most people do (calipers), its a bit apples to oranges. Additionally, store bough filament is generally rated at +/-0.05mm or +/-0.1mm, so you're right in the ballpark.

As for improving variation, reducing temperature and adding fan cooling should reduce variation, but the 2.1mm nozzle will be too large for that. 180C is recommended for ABS if filament diameter tolerance is the highest priority. Most folks have a little less drop in the loop, not sure if you've experimented with that while at the 33" apart.

13

Re: Any ideas how to have more consistent diameter in this setup

I had thought about the bearings, and put a mark on them to try and correlate the diameter oscillation to the bearing going round. I didn't observe any correlation, in my scientific eyeball test.

I had run a bit of store bought filament through and seem to remember the measurement being more stable. However, I never ran bought filament through and actually winding it on the filawinder.....

Will try that.

14

Re: Any ideas how to have more consistent diameter in this setup

Another thought - have you tried natural MG94 on this setup?

15 (edited by lboucher26 2016-03-30 02:00:17)

Re: Any ideas how to have more consistent diameter in this setup

I had put a fair amount of MG94 through it, but that was before I made the loop this large. I don't think the results were any better, but probably not much worse. Hard to tell, didn't have the thickness gauge setup yet.

Tonight i grabbed a spool of Taulman bridge, and another spool of purchased filament i had.
After initially being annoyed both rolls were at 1.7 nominal... instead of 1.75, I ran some through the filawinder thickness gauge setup. Probably 2-3 minutes worth. The general deviation matched what I as hand measuring and didn't do the oscillation. Total variation was probably +/- 0.3 and it kinda slowly meandered around, not large swings like I see when i extrude.

What I am most curious to see, is video of extrusion through other real time diameter monitoring setups (or copies of mine). I know there is a light based thickness sensor.
Really want to know if this oscillation is inherent to the vertical setup in general, or if its specific to my machine in some way.

Maybe their is something odd about the power getting to the motor, or the motor itself causing slight cyclical changes in motor speed.... I can easily monitor voltage... Should probably get the new motor controller board so i can see the current also... Any change in barrel pressure I would think would have a corresponding voltage/current change.

I will mention, now that I think about it.
Back when i was trying to fight PLA (kinda given up that fight for now.) I do remember seeing the barrel kinda walk around a bit, i think it happened when i was using too low a temp. It did stall once, but i was right their and stopped it. The nozzel end probably does still wonder a bit... Probably means my motor to barrel setup is completely straight, although I had thought it was kinda tolerant of misalignment since the coupling isn't rally rigid. Maybe it indicates something is bent... I will rig up a pointer or something so its easy to see how far the actual hole is drifting around while extruding. Wouldn't think it to matter much initially, but maybe whatever is causing the drift also causes a cyclical change in barrel pressure... And if barrel pressure is oscillating, that would explain diameter oscillation. All that said, the motor sounds consistently annoying, but bearably loud.

Im out of town next week for work, so its going to be a couple weeks till i get back to this.

Edit: Totally blanked, I already do have a voltage read out hooked up to the output of the PWM Board version 1. Voltage is stable. Maybe thats expected though, and i have to look at current.

16

Re: Any ideas how to have more consistent diameter in this setup

lboucher26 wrote:

Tonight i grabbed a spool of Taulman bridge, and another spool of purchased filament i had. Total variation was probably +/- 0.3

0.3? Sure about that?

17

Re: Any ideas how to have more consistent diameter in this setup

Sorry 0.03

18

Re: Any ideas how to have more consistent diameter in this setup

It sounds like the only other thing could be the pressure of the chamber/barrel as you mentioned above.  I would think this would this would cause slow oscillations as the pressure changes

19 (edited by lboucher26 2016-05-02 01:43:25)

Re: Any ideas how to have more consistent diameter in this setup

Hi All

So i finally got time to play with this setup again.
I got the new motor driver that displays voltage and amperage.
The amperage is fluctuating about .2 amps at the most.

How much fluctuation do other people see???

The fluctuation kinda sorta matches the fluctuation in diameter, buts its hard to really tell.
The nozzle does trace a small circle, its not much, maybe a few millimeters...

Without completely replacing the nozzle/barrel/mounting hardware, and replacing the wood body with a real metal body, i doubt i can get things aligned better...

Any other thoughts out there?

FYI, i did end up allowing the filawinder to stop, but its reaction is much much slower, which definitly helps it consistently it pull, and not start/stop so much and abruptly.

Here is video of the lastest setup.
https://youtu.be/HMHZV-eDhL4
Running 17V, i got out 700 grams, in maybe 7 hours, of colored PA 746.
Diameter is around +/- 0.5, good enough, that im about to give up on making improvements.

20

Re: Any ideas how to have more consistent diameter in this setup

I was seeing similar with mine last weekend and my thoughts with the pressure variations would be to move to a closed loop motor speed control, but in reality how far do I want to go?

Also thought of separating the motor power from the heater circuit as I noticed change in pitch when heater turn on/off.

21

Re: Any ideas how to have more consistent diameter in this setup

I added a second power supply for the motor a long time ago. Can't say I noticed any particular improvement, but I was changing so many things who knows. In reality, its so easy to add a second supply and most everyone has an old box full of power supplies, it can't hurt.

22

Re: Any ideas how to have more consistent diameter in this setup

Thickness oscillations are probably coming from those plastic bar guides, as any movement on the filament is transmitted back to the hot filament at the nozzle that is not yet cooled, the filament should hang in free air and make a gentle curve all the way to the spooler.

Also, keep the temperature cool:
When filament starts, it is thick because there is no weight to "draw" it out, as the loop forms, the weight increases so as the "draw" weight increases and then forms thinner filament which in turn decreases "draw" weight and causes it to thicken again.

You will end up with an oscillating thickness and lower temperature will help to minimize it.

I think that a "L" configuration would work better than a "U" but I have not tried it yet.

My 3mm set up:
My "U" config has 31" between winder and extruder, filament entry and exit at the same height, and a 20.5 inch drop to the laser
the PTFE tube starts at the bottom of the guide which is solidly mounted and has no flex and is looped in the direction of the extruder.