Topic: Stainless Steel filament
Got my stainless steel and magnetic iron filament today. Results.
Stainless Steel pla printed really well on an e3dv6. A fan is an absolute must. Found the sweet spot at about 230 c and the glass bed at 70 c. I started off trying no fan then half way through the print turn the fan on 100%. The fan being on is crucial with this.It didn't shine up as much as I had hoped yet. But then again I may not have the proper buffing pad for it but I'll enclose a pic.(the nozzle broke the little key chain part off my Marvin in the pic)
The magnetic iron actually printed better at a lower temperature. At 230 it wanted to bubble or ooze terribly bad. I found it to run best all the way down to about 208 C and the bed on 70 c.
The magnetism is great. I can put my magnetic Marvin upside down on any magnet and it will stick. It also shines up some where it has the iron in it.
Overall I liked them both and was pretty pleased after I made some adjustments. It's a little pricey but I think you get what you pay for.