miglo wrote:I dont know how you guys are getting 1kg in 8hrs. Just ran it for the first time this weekend and it took 25hrs to get 1kg of mg94.
Getting about 1.75 +/-. 07 at 186c.
Setup is vertical with a filawinder
Did you run it with the pound of material Tim sends first to flush out anything in the barrel after putting it together? If not, and that kilo was your first kilo, then I am going to guess that there are metal particles inside the barrel at the nozzle entrance that are blocking the nozzle. You'll want to heat the barrel and then remove power and carefully remove the brass nozzle and let it cool, then scrape, cut, or otherwise remove the plastic that will be stuck to the inside of the nozzle and you will see a ton of metal shavings embedded. Then, throw away that first batch of material because it probably has a ton of metal shavings inside it! After that, you will probably have no issues with blockages!
If that isn't the issue, then let us know!