What you describe has happened, though it is very rare - less than 1% of users report it. I think in your case either the barrel or auger were damaged by the initial problems, and need to be replaced. Either that, or during your reassembly the auger was not positioned properly in the barrel. Even industrial extruders are not supported on the nozzle end.
Here's what I know on users with similar problems:
Extrusion totally stopped:
elmoret (v1.3) - Problem happened after ~1500 hours of use, 95% MG94, 3% other ABS, 1% PLA, 1% ABS+black or green colorant. Prior to the clog, nothing my MG94 had been run for several hundred hours. Disassembled, removed plastic plug, reassembled. Problem has not resurfaced for ~200 hours since, extruding MG94 at temperatures from 180 to 190C. In the link, I detailed everything I observed - including the fact that after the barrel cooled, I could rotate the auger with a wrench - indicating the plastic was not even touching the walls of the barrel anymore. The jam occurred after heating up from cold - not after running for a period of time.
IanJohnson (v1.0) - problem happened after running Asaclean. Replaced barrel, problem did not resurface.
insta (v1.0) - problem happened after ~100 hours (5kg). Ran nylon pellets which seem to have pushed clog out.
digitydogs (v1.3?) Ran MG94 ABS and PLA for 200-500 hours, several jam/clean cycles to no avail. Two machines exhibit this behavior, two do not. One of the two exhibiting the jam ran GITD filament right before the jam, one of the machines that does not exhibit this behavior has run 50lbs of GITD filament.
kitcarguy (?) Ran GITD filament in the first few hours of use, jam occurred. Disassembled and cleaned twice, problem went away.
Very slow extrusion:
Ggalisky (v1.5)- Experienced 1-4"/min with MG94 and GP35 at 1.75mm diameter. Went up to 16"/min after clearing the clog, no issues since.
ericpaulbishop (v1.4) Experienced "dramatic slowdown", found that higher temperatures triggered it sooner, found that wrapping the barrel helped.
Slow extrusion, seemingly unrelated to this problem:
spencermatousek Experienced 6"/min at 1.75mm filament. Changed to 185C extrusion temps, jumped to 12-14"/min (normal). Probably a case of thermocouple/controller not well calibrated.
borreas Experienced 7"/min at 1.75mm filament. I made some suggestions, never heard back. Not sure if solved, but 7"/min is not characteristic of what we're discussing here.
wahada - experienced 4.5"/min at 1.75mm filament, in vertical configuration. Problem was poor pellet feed/hopper design/configuration, as confirmed here: http://www.soliforum.com/topic/6976/ver … er-shaker/ he is now achieving 30"min.
thormj Nozzle was blocked with debris, cleaned nozzle, problem went away. Now "very happy".
Hargert Barrel was not tight enough and rotated durign operation, blocking pellet feed.
That's what I'm aware of so far. That's 5 users with complete stoppages, and two with very slow extrusion which may be related to the same issue, for a total of 7. I also added some users who had troubles that were resolved by other issues - pellet feed, temperature, debris in nozzle, etc.