Just to demonstrate the affect temp and speed has on T-glase. Along with the difference between .40 and .60 nozzles.
Both of these are at .3 layer height.
This is the .40 nozzle running at 65 mm/s and the feedrate slider at 300. Temps starting at 245 and working down to 235 - 225 - 215 and 212 and no speed changes throughout the print.

This is the .60 nozzle running at basically the same settings with the exception that I slowed it way down where I have it marked. I wanted to do this in an area where the clarity was decent so I had to wait till I got to the lower temps.

Then just for easy comparison

Printit Industries Model 8.10 fully enclosed CoreXY, Chamber heat
3-SD3's & a Workbench all fully enclosed, RH-Slic3r Win7pro, E3D V6, Volcano & Cyclops Hot End
SSR/500W AC Heated Glass Bed, Linear bearings on SS rods. Direct Drive Y-axis, BulldogXL
Thanks to all for your contributions