So I’ll start by saying this is with a sample size of one per method which is rather poor, but it at least demonstrates which direction each solution can take, so don’t take it as read that any one method is the best as I’m sure you can understand a lot will depend on what level of smoothing you are trying to achieve and what model you are working with.
I have performed four different types of smoothing: A simple 5 second dunk in acetone, the vacuum chamber, acetone spray and heating the acetone (Presto Method).
Previously I mentioned about using an ultrasonic fogger to generate some smoothing but this turned out to be a bust straight away.
After getting everything set up I put the fogger in the acetone and nothing happened .
This was due to the level sensor built in to the fogger to make sure you didn’t run it dry. It used conductivity to sense the level and acetone isn't the same as water if you didn't know. However in the very short time it took to realise this was never going to work without building my own fogger the casing to the it had began to very quickly melt. I had to whip it out of the acetone and dunk it in water to try and stop the process before it fell apart, the housing had turned to rubber in about ten seconds. I might use this idea to get the electronics out of the housing yet, but at the time it was much more of a panic to try and save it. So anyway that idea was a none starter and I’ve left it alone for now.
For completeness as a comparison this is close up pictures of an unharmed frog



Starting with the simple 5 second dip:
As I had a jar of acetone and the frog fit quite nicely in the top a bit of copper wire around the poor thing was plenty good enough for a nice bath



That worked better than I expected, well once I realised that he was sticking to the surface I put him down on I manged to pull him up and let him air dry.
Next up was the vacuum chamber:
This is the setup I used with my hand pump.
And a quick one of him taking one for the team.

After a while I took him out, let him dry off and got these results



From the underneath picture you can see where the acetone did most of its work where the vapour has rushed in from the pipe which was directly below the model. The belly up to the throat is lovely and smooth. You can see some more subtle smoothing on his head and back. The whole model does have a gloss quality but the low resolution print was too much to over come in this case.
With a better print and a shield for the incoming vapour this could have had better overall results.
I have a problem going forward now as I've broken my hand vacuum pump, so need to get a proper electric version if I am going any further.
I then moved on to using an acetone spray via an airbrush. I had one that came with an old compressor but figured it was going to be designed for use with solvents so it should hold up well and most of the parts that touch the acetone are made of brass.
There was general problem with this though. As I had to use it outside the fine spray of acetone was just able to make the model wet before it dried so even though I tried for a while it didn't give very good results at all, leaving the model with a matt finish, although this could have been some contaminant in the airbrush as I had never used it before.



Finishing off I used a rice cooker that seems to be as close to the Presto cooker I could find in the UK at a cheap price.
I ended up with this...



I think you can see that the model is much smoother than previous methods. You can just make out some marks on the belly where the frog started melting so quickly that I had to loop some wire around him and pull him off the tray it was sitting on but by then he was stuck so I ended up getting the wire stuck to him.
This was my fault for underestimating how quickly this would work, next time I will try for a much shorter period before turning it off and getting him out to dry.
Some observations:
If you want to smooth more make sure air doesn't get to the model. Once the air is let in everything start to solidify quickly and although it doesn't harden for quite some time the smoothing process stops very quickly.
Using any method can get decent results if you keep trying and work around any issues you find.
Acetone isn't as dangerous as everyone seems to try and make out. Whilst airbrushing the frog I thought I would see how flammable the spray was and got a lighter out. The spray would just put the lighter out every time. So thinking the flame wasn't hot/big enough I got a blow torch out and found that just air would interfere with the flame as much when the acetone was coming out.
Now I won't say it is safe, clearly it is flammable, but when using the Presto method I just had it on a window sill with the window open. I can't see any possibility of any harm coming from that. If you are a smoker probably best not to smoke around it though.
Sorry for the long post, I tried to trim the pictures to the bare minimum, I had 160MB to start with. 
For now I will be using the Presto method as it is easy, but I need to get a timer to get better control of it.