1 (edited by dubbsd 2020-06-09 22:46:10)

Topic: PETG did not stick to bed

I am using PETG and it let loose from the bed I have had it pull chuncks out of the glass where their was not glue
But it has never let loose. I am printing with glass and glue stick. bed temp  80°c using a .8 printcore. nozzle temp  240°c
printing at .24 layer thickness 2 shells
the part is aboyt 4" in diameter so it had a lot od area on the bed.

Thanks
Dale
http://soliforum.com/i/?mhnC45z.jpg

Ultimaker S3.

2

Re: PETG did not stick to bed

Use hairspray. Aquanet is cheap and one application is good for several prints. Also make sure the first layer is not as squished as you would for PLA or ABS. Instead of half of your desired layer thickness you want the squish to only be about a third.

Printing since 2009 and still love it!
Anycubic 4MAX best $225 ever invested.
Voxelabs Proxima SLA. 6 inch 2k Mono LCD.
Anycubic Predator, massive Delta machine. 450 x 370 print envelope.

3

Re: PETG did not stick to bed

Thanks Carl

Ultimaker S3.

4

Re: PETG did not stick to bed

You want the Aqua Net in the purple can.. "Extra Super Hold" variety.. have been using this stuff for years..

Light mist coats - 2-3 - spray on one, let set up with bed at 60C, spray next... do not pile it on.

Protect the moving parts & hotend with something.. drape rags over, block with cardboard, etc. If you have a removable bed.. take it out to spray.

SD4 #1 & #2 - Lawsy carriages, E3D v6, Rumba controller board, mirror bed plate, X motor fan, upgraded PSU & Mica bed heater
SD4 #3 - in the works ~ Folgertech FT-5, rev 1
Printit Industries Beta Tester - Horizon H1

5

Re: PETG did not stick to bed

A 4-inch diameter part has a lot of surface area, which means it generates significant shrinking forces (warping) as the upper layers cool. This force is what's pulling your print off the bed.  In your slicer, set the part cooling fan to 0% for the first 3-5 layers. After that, have it ramp up slowly to a maximum of 30-50%. Never 100% fan for PETG unless you are doing extreme bridging.