Topic: Bulging at bottom of part?
Since switching to repetier i was having annoying problems with bulging in the first 5-10 layers. I was constantly messing with my bed leveling and do offsets to my z and really not getting anywhere.
Then i noticed what the problem was, in the custom gcode of slicer it had:
G1 Z5 F5000;
I guess this was added as a clearance in the event your bed leveling was really off.
Unfortunately what this did was introduce backlash into the first bit of the part until the slack was taken up since these machine use a standard threaded rod vs a ballscrew.
So i replaced that code with:
G1 Z-1. F5000 ;
G1 Z0. F5000;
Which moves the bed up past 0 1mm then back down to 0 to take up the backlash. Results below, before change on left after on right. I figured i would post incase anyone else has this issue.